5.2.1 Point Defects | |||||||||||||||||||
5.2.1 The Gang of Four | |||||||||||||||||||
| We start with zero-dimensional defects; the smallest denizens of the defect zoo. Here they are - all four of them: | |||||||||||||||||||
| |||||||||||||||||||
| It's pretty simple. More than those four "point
defects" we cannot make by playing with atoms inside an elemental crystal,
meaning a crystal made from just one of the elements like iron or silicon. The question we need to answer now is "why" and "how many"? Why should a crystal contain those defects and if there is some reason, how many should it be? | |||||||||||||||||||
| Well, we already know that any crystal can and will make vacancies because it needs to produce disorder to achieve nirvana. If you glimpse ahead a little bit, you can see how the crystal makes vacancies. | |||||||||||||||||||
| For exactly the same reasons creating increasing disorder with increasing temperatureit also can and will make "self-interstitials", atoms of its own kind that squeeze themselves into the interstices or interstitial positions in the lattice. | |||||||||||||||||||
| The first question thus finds an easy answer for two of the four point defects. We are left with figuring out how many vacancies and self-interstitials we must have at some temperature. | |||||||||||||||||||
| Disorder is more important at high temperatures. This can only mean that the
number or the concentration of both vacancies and self-interstitials must
increase with increasing temperature. If you bothered to look at the science
module about vacancies, you know that the concentration increases exponentially.
If you didn't, you may want to check the "science" module to get some idea what "exponential
growth" means. Just a hint: If you hate exponentials and logarithms but like money, you should reconsider. It's those dreaded math objects that will tell you how your money will go down the drain with the coming inflation (or through the roof if you invest it wisely). |
| ||||||||||||||||||
| OKfor those of you who can't overcome their fear of math: Exponential growth of the vacancy concentration with temperature means that the concentration goes up rapidly with temperature. Here is a calculated curve showing the approximate vacancy concentration in iron as a function of temperature: | |||||||||||||||||||
| |||||||||||||||||||
| So, yes, the concentration is indistinguishable from zero over most of the temperature
regime. Only at rather high temperatures it goes up rapidly. That doesn't mean that there is nothing at lower temperature,
you just can't see it in this plot. If you plot the total earnings in your country versus time, your salary of 2.654
(or of whatever you currency might be) this July will simply not show eithereven so it was very
meaningful to you. In the science module you can look up how to make better plots of vacancy concentration. | |||||||||||||||||||
| OKnow you know more about vacancies than you ever fancied in your wildest dreams. How about self-interstitials? | |||||||||||||||||||
| It is exactly the same thing. Self-interstitials do the same thing as vacancies:
they introduce disorder and thus raise the entropy. They just don't do it quite as well as vacancies in almost all common
crystals. Most crystals, including all metals, therefore prefer vacancies to self-interstitials by far, and only make a tiny amount of self-interstitials that we can simply forget about. Iron self–interstitials thus are completely unimportant to sword making and we won't mention them ever again (except in the science module). |
|||||||||||||||||||
| The big exception, by the way, is Silicon (Si). In silicon crystals the self-interstitial is of major importance. How that was found out and drummed into the heads of the non-believers, would be a long story of its own. I'd love to tell it because I had a hand in it. I will restrain myself herebut not in this link. | |||||||||||||||||||
| The vacancy and the self-interstitial are the two zero-dimensional defects that
we subsume under "intrinsic point defects" for obvious reasons. "Intrinsic" is one of those fancy Latin words we scientists like to use in order to show
off. It means "innate", or "incarnate" in the sense that the crystal needs nothing from the outside
for making themin contrast to the extrinsic (extraneous, foreign) point
defects shown on the right in the figure above. So let's look at the two extrinsic guys now, some foreign atom in an interstitial position, or some foreign atom at an substitutional position. We also call them impurity or dirt atoms, and sometimes doping atoms or alloying elements, I'll come back to that. | |||||||||||||||||||
| I know. Those names suck. If you can come up with better ones, let me know. And
while you are at it, find better names for other outlandish expressions like: democracy, republicans, maitre'de, caucus,
anonymous, dermatologists or ophthalmologist, too. Or simply accept that it's not worth the bother to rename things that
already have good working names, however weird. All our intrinsic / extrinsic / interstitial / substitutional stuff is reasonably
clear and you got to have some names, after all. If you could live with things having names like "George Walker Bush", you shouldn't have a problem with dirt going by the name "substitutional foreign atom" either. |
|||||||||||||||||||
| As far as dirt is concerned, foremost on our mind is of course In silicon, carbon would be a substitutional foreign atom, replacing ("substituting") one of the silicon atoms, so it depends on the host crystal which of the two possibilities a given foreign atom will assume. Let's summarize: |
|||||||||||||||||||
| |||||||||||||||||||
| When we talk about carbon in iron, we usually consider concentrations between 0 % and 1,5 %. Those are always weight percent (written wt % if you want to be precise) if not otherwise stated (remember?). | |||||||||||||||||||
| This makes a lot of sense in material engineering
because you can easily make desired mixes by weighing the ingredients. In materials science, however, we look at atoms. In order to assess foreign atoms in a host crystal, we need their concentration in atom percent (at %). In other words, we want to know how many percent of all the atoms present are carbon atoms? There is no easy way to switch from one to the other; consult the link for how it's done. |
| ||||||||||||||||||
| If we take, for example, the "magical" 6.7 wt % of carbon and express it in atom percent, we get 6.7 wt %=25 at %. A quarter of all atoms then are carbon atoms. Why 6.7 wt % of carbon of carbon is "magical" we will see laterbut you are welcome to make a guess, now that you know it corresponds to a mix of iron : carbon=3 : 1 in terms of atoms. Hint: one could write that Fe3C. | |||||||||||||||||||
| What a schematic iron crystal would look like with 1.75 at % (» 0.3 wt %) or 5 at % (»1 wt %), respectively, of carbon atoms dissolved in the volume of the iron, is schematically shown below. | |||||||||
| |||||||||
| You are looking at a virtual cut through the crystal, of course, and at any plane
inside the crystal it would look like this, just with the carbon atoms distributed at random at interstitial positions.
We also call this "the carbon is dissolved" or it is in solid
solution. Now why should that be virtual? I stated some time ago that there are special microscopes that allow you to look at the surface with atomic resolution. Yesbut: If we look at a real surface of almost anything you wouldn't see much because a real surface of almost all crystals in air is oxidized. With an iron sample you always would look at "rust", even if to your eye it looks bright an shiny. An iron oxide layer just a few atoms thick, totally invisible to the eye, is all it takes to completely obscure a surface from atomic "view". | ||||||
| Even if we use the common (and expensive) technique of putting our sample in ultra-high vacuum (UHV) where it can't oxidize, and "somehow" take off the original rust layer in there, we would still have a hard time seeing anything! Why? Because iron is magnetic! That tends to mess up many microscopes, including the STM we would need to employ here. I have therefore no iron surface pictures taken at atomic resolution that looks remotely like the schematic picture above. The best I can give you are pictures of point defects in a gallium arsenide (GaAs) surface. | ||||||
| Note that despite the rather small weight percent
concentrations of about 0.3 wt% or 1 wt%, respectively, in the figures above, it's actually quite
a bit of carbon if you think about it. Nevertheless, most "bonding springs" still connect iron atoms
and thus Young's modulus is hardly changed
relative to that of pure iron. Note that this not a theoretical prediction open to some doubt. This is as hard a fact as you like them to come. |
||||||
| Now that we have played around a bit with an extrinsic
defect like carbon in iron, the same question as above for the intrinsic defects comes
up: Why should a crystal contain those extrinsic defects, and if there is some reason, how many should it be? |
||||||
In an ideal
crystal world the answers to those questions would be exactly the same as for
intrinsic point defects:
| ||||||
| In an ideal world you would have the proper amount of money necessary for achieving your personal nirvana conditions. But neither you nor the crystal exist in an ideal world. A crystal cannot make foreign atoms at will, just as (most of) us cannot print money all that easily. | ||||||
| So in the real crystal world, the answer to these questions is different from the one describing the ideal word. It is extremely simple but will have formidable consequences: | ||||||
| ||||||
| Tough luck. The number of any atoms forming
extrinsic point defectsinterstitial carbon in iron, substitutional carbon in silicon, substitutional phosphorous in
iron, ..., (the list here would contain about The crystal can neither make more foreign atoms or impurities if it wants too, nor can it easily get rid of the ones it has. It needs a little bit of help from friends like you for this task The consequences are dramatic: |
||||||
| ||||||
| Our steel blade or crystal with 0,5 wt% carbon in it, or just any crystal containing
impurities, is stuck now. It wants to have a certain precise number for nirvana but chances are extremely high that the
number it actually has is far off that nirvana number. The crystal is stuck. What is it going to do? |
||||||
| Exactly what you would do if your 9 children are running all about the place, producing far more disorder than needed, and keeping you from achieving you preferred state of being (easy chair, peace and quiet, good wine, a good book like this one). You round 'em up and lock them into a room somewhere else. Crystals do the same thing; they imprison their impurity atoms or, as it is properly called, precipitate them. We will see how that works shortly. But before we do that I want to generalize a bit. | ||||||
| It should be clear that as far as extrinsic point defects go, we are not restricted
to carbon. I can take whatever else the periodic table has to offer (about 90 elements) and put it into my iron. I know
how to do it in reality, for you it's an easy thing to do in your brain lab. Now let's look at how these impurities have settled in the iron. The good news is that the foreign atoms can assume only three different configurations: | ||||||
|
||||||
Let's look at few examples
|
||||||
| Which elements we have inside the iron crystal, how many, and in what kind of configuration determines most of the important properties of your steel. | ||||||
| So, without a little bit of help, the concentration of extrinsic
point defectsimpurities in crystals won't change, in contrast to the intrinsic
point defects that the crystals can make and dispose of on its own. This is great because that's where you and I come in. If you know how to do it, you can change the impurity concentration of a given crystal, no matter if the crystal likes it or not. That's where technology starts. Let's look at two examples: | ||||||
| Building a silicon microprocessor or most anything else from silicon
(Si) needs to start with a very clean and perfect silicon crystal, as close to nirvana as it can be. This involves producing
extremely clean liquid silicon first. In a second step an almost perfect crystal is grown by rather involved methods. Then we mess up the crystal by putting substitutional impurities like phosphorous (P), arsenic (As), or boron (B) inside well defined parts of it. So the concentration of extrinsic point defects does change: it goes up. The crystal doesn't like it, of course, because that takes it rudely off his near-nirvana state of being. It fights back in many ways, and it fights dirty! That is one of the reasons why microelectronics technology is not a simple enterprise. |
| |||||
| When we make steel in modern times, we start with rather dirty liquid iron, it is actually cast-iron. We remove most of the unwanted dirt already in the liquid state and we add some wanted dirt. Crystallization is not controlled on a microscale so we get (huge) polycrystals. Certain processes in the solid crystalline state (like "case hardening") will change the concentration of some impurities (mostly carbon) to some extent. | ||||||
| One last word to impurities in crystals. Without going into more details, one thing becomes clear: it is far easier to mess up a crystal then to keep it clean or to clean it up if its messy. It's not so difficult to get impurities inside. Crystals, after all, like to have some at high temperatures. It is just far more difficult or well-nigh impossible to get them out again. | ||||||
| It is just the reverse of opening a can of worms, or squeezing tooth paste or your heir out of a tube. The problem there is to get the stuff back in. | ||||||
© H. Föll (Iron, Steel and Swords script)