5.4 Weird Denizens of the Defect Zoo |
||||||||||||||||
5.4.1 The dislocation | ||||||||||||||||
| I can no longer avoid to introduce you to one-dimensional defects. There is only one kind: the dislocation. | ||||||||||||||||
| A dislocation, when you first meet one, appears to be rather fascinating but weird. You don't know how to handle it, what it is good for, and what to do with it. It's just like a new-born baby. So let's just make one (a dislocation, not a baby). That's relatively easy, even if you don't know exactly what goes on during the first few tries. Go through the moves a few times, and you will get the drift, just like - well you also get this drift. | ||||||||||||||||
| First we look at a schematic drawing of a three-dimensional perfect crystal as shown below. It's schematic because I spared you (and me) all the atoms inside the crystal. It's also a cubic primitive element crystal that doesn't really exist but is easy tro draw. Since just showing atoms is a bit confusing, I also indicate some particular planes in blue. | ||||||||||||||||
| ||||||||||||||||
| We put our model crystal into a vise and now press like crazy
on the upper right hand part. Bang it with your hammer if you like, but the stress distribution generated in this way tends
to be a bit messy (the red arrows would have different lengths and would not be exactly at right angles to the crystal plane)
. Essentially we want to move or shear the upper part of the crystals somewhat to the left. If enough force, pressure, bang, or to call it by the correct name: stress is exerted on that outmost plane of atoms, it will eventually do an interesting thing as shown in the next picture of our little comic strip: | ||||||||||||||||
| ||||||||||||||||
| The outermost plane with all the atoms on it is squeezed so much to the left that it eventually squeezes the neighboring planes of atoms so much to the left that the bonding between one row of atoms snaps. The outermost plane takes the part of the second plane, bonding with the atoms below. The second plane then ends inside the crystal. | ||||||||||||||||
| ||||||||||||||||
| To be more precise, we have generated a particular kind of dislocation, called
an edge dislocation. If we keep pressing, the dislocations moves. The ending plane of atoms joins up with the plane next to it and thus moves deeper into the crystal. The animation shows that schematically, but be aware that this happens all along a line at right angles to the screen.. What an edge dislocation deep in a crystal finally looks like is shown below in a thee-dimensional rendering . | ||||||||||||||||
| ||||||||||||||||
| If we keep pressing, the dislocation will move all the way from left to right,
finally emerging on the right (look at the animation). The net result is that the upper part of the crystal has been displaced
relative to the lower part. In other words: | ||||||||||||||||
| ||||||||||||||||
| In yet other words: We have moved a big objecthalf a crystalnot in
one fell swoop that would have required to break a lot of bonds and thus a lot of energy, but step-by-step, with rather
little effort. We have sheared off the top relative to the bottom and that's why we call that kind of deformation a shear deformation, the kind of deformation you get when you exert force parallel
to a surface. Dislocations can only produce shear deformations and never what we call normal deformations, the kind of deformation you get by pressing normal to the surface on things. This link illustrates and explains that in more detail. | ||||||||||||||||
| Mother nature, of course, has discovered the principle of moving big objects the easy way long ago and implemented many variants of that basic principle. | ||||||||||||||||
| In our case we want to move the whole top of the crystal to the left.
The idea is not to move the whole body with brute force, but only small parts of it at any given time with far less effort.
To say it a bit differently: Localize a certain deformation in a small part of the body and then move that "defect" through the body. The following pictures show this principle for two biological objects and a man-made object (big rug). In all cases it is far more efficient to move a "fold" through the object than the whole object. In crystals, dislocations do just that. | ||||||||||||||||
| ||||||||||||||||
| Crystals knew all along, for the better part of 10 billion years, that life with defects like dislocations is much easier than being perfect. | ||||||||||||||||
| Humans, however, did not figure out that dislocations are absolutely essential to sword forging before 1934; we shall see why in a moment. About 3.000 years had to pass for iron technology, and far more for general metal technology, before we first understood what was going on when "bending" a metal. Dislocations are not only essential for sword forging but for all the bending done by the "metal bending industry, as we call our still largest and most important industry. Compare that to the first "use" of electricity by Volta around 1770, and a full-fledged industry based on an almost complete understanding of electricity around 1900. | ||||||||||||||||
| Dislocations are also extremely important for most of semiconductor electronics because there you must not have them! Since you can only avoid something if you know what it is, silicon technology would be impossible without a thorough knowledge of dislocations (and other crystal lattice defects), including how one can avoid having any in the silicon wafers one starts with, and how not to produce them during processing. | ||||||||||||||||
| Nevertheless, lots of peoples missed the big moment when Taylor, Polyani and Orowan discovered dislocations in 1934. | ||||||||||||||||
| Worse, it took even until about 1960 before dislocations became common-place in
scientific and engineering circles. The big breakthrough was the invention of the transmission
electron microscope (TEM). Do you know who invented it? I thought so. Go to this link. Do not collect 100 Dollars. Anyway, since about 1960 one could see dislocations, and seeing is believing. | ||||||||||||||||
| I will allow that a lot of people were a bit distracted beeen 1930 - 1950. Some other events like the Second World War happened in this period of time and no Noble prizes were awarded. After the war, lots of Nobel prizes went to the heroes of atomic and nuclear science who unveiled major secrets of nature and produced atom bombs on the side. That was fine. It is nevertheless inexcusable that no Nobel price was ever awarded to the scientists who dug down to the very roots of mankinds most important technology. | ||||||||||||||||
| The Nobel price committee tried to make up for this oversight by awarding a Noble price in 1986 to Ernst Ruska
(1906 - 1988). He was one of the heroes around the invention of the electron microscope and in 1986 the only
survivor from the heroic times when dislocations and other defects in crystals were discovered and we finally understood
what is going on inside a metal when you bang it with a hammer or work with it in any possible way. So if you, like me, haven't been awarded a Nobel price so far, you are in very good company. The special module gives you an idea of the people who were instrumental for understanding sword forging. |
| |||||||||||||||
| Just to make sure, let's look once more at how dislocations achieve plastic deformation in a schematic way. | ||||||||||||||||
| ||||||||||||||||
| We produce a dislocation by pressing as shown below (or above); next it moves through the crystal. When it emerges on the other side, the total effect is that we moved all the atoms in the upper part of the crystal with respect to the lower part by one atomic distance. As long as the dislocation is still inside, only parts of the upper half has moved. | ||||||||||||||||
| Did bells ring in your brain? Did you note the magic word? Here it is: "we moved all the atoms". We moved atoms with a dislocation! Moving atoms, I'm sure you will recall, was at the root of changing something in a crystal and that was the key to changing properties. The magic word was diffusion, or the random movement of atoms by some mechanism. With a dislocation we move a lot of atoms too, but pretty much in lockstep, the exact opposite of random atom movements in a diffusion process. We shall call this kind of moving atoms around a military movement. Moving atoms around individually and at random by diffusion, we then shall call a civilian movement on occasion. |
||||||||||||||||
| The dislocation itself is the region where things don't fit anymore. It is a line defect, with an extension in just one direction. Along the dislocation line, atoms would not see their usual environment, so we have a one-dimensional defect. |
| |||||||||||||||
| There is far more to dislocations than I can relate in this introductionary subchapter. The (two) science modules give a small taste treat of some of the more elementary stuff encountered when looking a bit closer at dislocations. | ||||||||||||||||
| Now get ready for the climax! | ||||||||||||||||
© H. Föll (Iron, Steel and Swords script)