A piece of paper has a fairly flat surface but you can see it
from all directions. Why? Clouds are formed by condensed water in the atmosphere and you can cleary see them radiantly white
against a blue sky. Why? Before you answer, consider that you can't see the uncondensed
water vapor even so the water concentration is about the same as in the cloud. And why, exactly, is the sky blue? Why is
milk (= water with a few percent of fat) white but water with a few percent of alcohol colorless and transparent? Even if
it contains far more than a few percent of e.g. alcohol? |
|
 |
The answer to the first question should be obvious. Even if the reflection law
is fully valid for white paper, i.e. ain = aout,
every pixel of it is normally hit by light coming from all direction so some of it will
always be reflected right into your eye. |
|
 |
Sure. Now go and shine a Laser beam on a piece of paper in an otherwised completely dark room
and you will still see the paper, no matter from which direction you look at it. Obviously
some of the Laser light is still scattered into your eyes even so the beam reflected
from its general surface goes somewhere else. Why? Because the paper is not really or
optically flat. Some parts of it always reflect light in the direction you are looking. |
 |
We are now looking at the interaction of light with matter of not-so-perfect properties,
especially at matter with properties that change on a small length scale. |
| | |
|
| |
 |
The paper, for example, is not perfectly flat but has a roughness on some length
scale far larger than the wavelength of light, but smaller than what your eye can easily resolve as shown in the picture.
Some parts of it thus are always reflecting the light into your eye. |
| | |
 |
Condensed water vapor means you have small water droplets suspended in the atmosphere
(if they're too big, they fall down and we call it rain); milk means you have some small emulgated grease particles in the
water. |
| |
| |
 |
Light is scattered at those small things in all directions
and the scattering of light is one topic we encounter if we look at not-so-perfect
materials |
| |
|
 |
Since "small"and "large"are relative values we must use the
obvious natural length scale when dealing with light as our ruler and that is of course the wave length l
» 1 µm. We then distinguish three cases depending on the length scale lmat
inherent to our material |
| |
| |
|
- lmat << l: The extreme case would be scattering at single
atoms or molecules. Proper nanoparticles also belong into this group.
This kind of scattering is called Rayleigh
scattering.
- lmat >>l: No problem, we covered that already. Just look at
any part of the sample by itself, apply what we discussed before, and then add up across the sample
- lmat »
l: Now we have a problem. What will happen in this case is difficult to deal with and no
general rules apply. This kind of scattering is called Mie
scattering.
|
| | |
|
 |
It is clear that the relative magnitudes of both reflection types depends on exactly
what the surface looks like at a small scale, and that one could have all kinds of reflected intensity distributions vs.
angle. It is thus convenient to characterize a surface (for a given wave length) by polar diagrams as shown below |
| |
|
|
 |
An "optically" smooth surface scatters
only little light outside the specular reflection direction, a perfectly rough surface scatters evenly in all directions,
producing a polar diagram that can be typically described by I = I0cosa.
|
|
 |
It is clear that "optically smooth" means that all deviations from the average perfect
surface, i.e. all quantitative roughness parameters, must be substantially smaller than the wavelength of the light considered. |
|
 |
If we take optics to the extreme, e.g. with DUV or EUV (= deep or extreme ultraviolet)
lithography with wavelengths down to the 20 nm region, we need to use mirrors for reasons discussed
before. Those mirrors need to be large (numerical aperture
is important) and flat to atomic dimensions! Not so easy to make and calibrate! |
| |
|
|
Transparency, Translucency, Opacity |
| |
|
|
Now let's look at light beams transmitted through a not-so-perfect but basically
transparent material. Those materials, by definition, have a small k value, i.e. a small
imaginary part of the complex index of refraction or, same thing, of the dielectric function. |
|
 |
As shown in the picture, we have
- Specular and diffuse reflection at the surface the light is impinging on. This is descirbed by the polar diagram characterizing
this surface.
- Scattering of the transmitted light (running in different directions) at defects or imperfections contained in the material
(fat droplets in milk, air bubbles in glass, ...).
- Specular and diffuse reflection at the internal surface the light is coming out off. This is described by a (different)
polar diagram characterizing this surface.
|
| |
|
|
 |
If your material is not fully transparent (i.e. looking
through it you hardly notice it is there; for example optical glass), light will come out in all directions and we call
it translucent, for example etched glass or milky glass. If a lot of the light is refelcts
and absorbed internally, nothing much will come out at all and we call this material opaque,
for example china ware or "milky" ice. |
 |
Of course we can put some numbers on the properties transparency,
translucency, and opacity, but we will not do that
here. |
|
 |
Suffice it to say that good transparency is a rather rare property -even for materials with
intrinsically small k and thus little absorption. Most ionic crystals and oxides, e.g.
Al2O3 are perfectly transparent as ideal crystals; this is also true for many polymers. Your
chinaware and almost everything else made from those materials, however, tends to be rather opaque and at best somewhat
translucent if it is thin. |
|
 |
The reason are imperfections of surface and in the bulk of the material. Any defects not far
smaller than the wavelength of the light will make their presence felt by scattering some of the light in unwanted directions. |
 |
Metals are also rather opaque but for a different reason. Since their free electrons
can absorb arbitrary energies and momenta, incoming photons quickly find a suitable electron that will "take"
their energy and momentum, "absorbing" the photon within a few nanometers below the surface. |
|
 |
Scattering or no scattering - nothing will come out on the back surface in either case. |
 |
The picture above contains a small puzzle - did you notice? |
|
 |
The main beam is drawn nicely refracted at the air - material boundary. For doing this you
need an index of refraction for the material. What is the index of refraction for an optical
compound material? The question is reminescent to, e.g., Young's
modulus for compound materials. |
|
 |
The answer, not unexpectedly I hope, is: As long as the constituents of the compond are small
enough, it is possible to define a compound index of refraction that is a weighted average of the individual indexes. |
|
 |
Eaxtly how you do this might be tricky but there is nothing special here. |
| | |
|
|
Rayleigh Scattering |
| |
|
|
Why is the sky blue? Because the air molecules
scatter blue light stonger than red light. |
|
 |
So if you don't look at the sun directly, only scattered light scattered somehow
in the atmosphere can reach your eye. The more you look in a direction away from the sun, the bluer the light will be. Actually,
it should be violet but because the eye is not very sensitive to the shortest still visible wave lengths you are biased
towards blue. |
 |
Atoms and molecules are far smaller than the wave length of light so we are talking
Rayleigh scattering here. In contrast to Mie scattering occuring for
particles with sizes comparable to the wave length, Rayleigh scattering can be treated analytically. Here we only look at
the major points of this treatment. |
|
 |
The figure shows the basic situation. An incoming light beam in the form of a plane wave with
some energy or intensity (per cm2) is transmitted to some extent and scattered to some other extent. We
assume that scattering happens evenly in all directions, symbolized by the spherical wave emanating from the atom / molecule. |
|
 |
In the particle pictures, a stream of photons with some flux density or power per cm2
and second hits the atom / molecule. A given photon is either not affected at all and just continues going straigtht, or
deflected (= scattered) into some other directions with equal probabilities for all directions. |
| |
|
 |
If we relate the total power (= energy per second) Psc
contained in the scattered part to the intensity I = power per cm2 contained in the incoming
beam, i.e. from Psc/I = s, the quantity s
has the dimension cm2 and is therefore called the scattering cross
section. |
|
 |
It is easy to understand the meaning of the s. The energy
or the power contained in the incoming beam that flows through an an area of s
cm2 is what will be scattered out of it. |
|
 |
We might expect that s scales roughly with the (two-dimensional)
size of the scattering particles, i.e. we expect it very roughly to be found in the 10–19 cm2
region. |
 |
Why does an atom / molecule scatter light? |
|
 |
Read up chapter 3.3.3 and you
know. The electrical field of the incoming wave jiggles the electrons of the particle ("electronic polarization").
Accelerated electrons (that's what jiggled electrons are) emit electromagnetic radiation (= light) with the frequency they
are jiggled with, which is the frequency of the incoming light. The total effect is the scattering of the light. |
|
 |
Looking a bit deeper into the characteristics of radiation emittance of jiggled electrons
(the word "antenna" comes up in this context if we look at it wiht electrical engineers eyes), one finds that
the power radiated into space scales with w4 or l–4.
Going through the math for a particle with volume V one obtains |
| |
|
 |
If we have density of n particles (= atoms / molecules / whatevers)
per cm3, we can estimate the penetration depth or absorption length lsc; i.e.
the length after most of the incoming radiation has been scattered off and nothing comes out anymore, to |
| |
|
|
 |
This calls for an exercise |
| |
|
| | |
|
|
A Bit More to Scattering
|
| |
|
|
We have now dealt with most of the questions from
above directly or indirectly: |
|
 |
A piece of paper has a fairly flat surface but still you
can see it from all directions. Why? Because it is far from being optically flat
and we have diffuse reflection and not just specular
reflection. On top of that we might have some Mie and Rayleigh scattering at the small and very small inhomogeneities. |
|
 |
Clouds are formed by condensed water in the atmosphere and you can clearly
see them radiantly white against a blue sky. Why? - considering that you can't see the uncondensed water vapor even so the
water concentration is the same.. We have Rayleigh scattering at the small water droplets and since the scattering
cross section scales with V2, small water particles containing n water molecules
scatter the light far more strongly than n water molecules far apart. |
|
 |
Why, exactly, is the sky blue? Because Rayleigh scattering increases
sharply (fourth power) with decreasing wave length. It is blue and not violet because the sun emits more blue than violet
photons and our eyes are more sensitive to blue than to violet. |
|
 |
Why is milk (= water with a few percent of fat) white but water colorless
and transparent? Even if it contains far more than a few percent of e.g. alcohol? See above. |
 |
One last point needs to be made. If we consider large
water droplets or simply a pool of water (huge droplet), it doesn't seem to scatter light very much. If the surface would
be perfect (consider a perfect ice crystal for the sake of the argument) there would be some perfectly specular reflection
but nothing else. Why? |
|
 |
The reason is that for Rayleigh scattering from water droplets far smaller than the wavelengths,
the electrical fields of the waves coming from each of the n water molecules of a small droplet have all pretty
much the same phase. The phases of the scattered waves from randomly distributed molecules then are random, and you know what that means.), so it is small wonder that scattering increase with volume
or number of molecules squared. |
|
 |
If the droplets get larger we first enter the (difficult) regime of Mie scattering and we
don't know off hand what we are going to see. For really large volumes, e.g. a visible ice crystal, we know what we will
see. however. What has changed now is that for any wave send out by some atom at the surface via scattering on some direction
other than the direction of specular reflection, some other atom at the surface produces an identical wave but with reversed phase. So all intensities cancel - except in the specular reflection direction. |
|
 |
The transmitted light cannot be scattered at all at the atoms of a perfect crystal (or "liquid").
Only imperfections like small precipitates or voids in crystal or fat globules in milk will scatter. |
© H. Föll (Advanced Materials B, part 1 - script)