First Task: Derive numbers for the mobility µ. |
|
 |
First we need typical conductivities and electron densities in metals,
which we can take from the table in the link. |
|
 |
At the same time we expand the table a bit |
| |
| Material |
r [W cm] |
s [W1 cm1] |
Density d × 103 [kg m3] |
Atomic weight w [× 1u = 1,66 · 1027 kg] |
n = d/w [m3] |
| Silver Ag |
1,6·106 |
6.2·105 | 10,49 |
107,9 | 5,85 · 1028 |
| Copper Cu |
1,7·106 |
5.9·105 | 8,92 |
63,5 | 8,46 · 1028 |
| Lead Pb |
21·106 |
4.8·104 | 11,34 |
207,2 | 3,3 · 1028 |
|
 |
For the mobility µ we have the
equation |
| |
|
 |
With q = elementary charge = 1,60 10–19 C
we obtain, for example for µAg |
|
|
| µ | Ag = |
6,2 · 105 1,6 · 1019 · 5,85 · 1028
| |
m3 C · W · cm |
= | 66,2 | |
cm2 C · W |
|
|
 |
The unit is a bit strange, but rembering that [C] = [A · s] and [W] = [V/A], we obtain |
|
|
| µAg | = | 66,2
| | cm2 Vs |
| | | |
| | | µCu
| = | 43.6 | |
cm2 Vs |
| | | |
| |
| µPb | = | 9,1 |
| cm2 Vs |
|
|
 |
Second Task: Derive numbers for the drift velocity vD by
considering a reasonable field strength. |
|
 |
The mobility µ
was defined as |
| |
|
 |
So what is a reasonable field strength in a metal? |
|
 |
Easy. Consider a cube with side lengt l = 1 cm. Its resistance
R is given by |
| |
|
|
 |
A Cu or Ag cube thus would have a resistance of about 1,5 ·10–6
W.
Applying a voltage of 1 V, or equivalently a field strength of 1 V/cm thus produces a current of I
= U/R
» 650 000 A or a current density j = 650 000 A/cm2 |
|
 |
That seems to be an awfully large current. Yes, but it is the kind of current
density encountered in integrated circuits! Think about it! |
|
 |
Nevertheless, the wires in your house carry at most about 30 A (above
that the fuse blows) with a cross section of about 1 mm2; so a reasonable current density is 3000 A/cm2,
which we will get for about U = 1,5 ·10–6
W · 3000 A = 4,5 mV. |
|
 |
For a rough estimate we then take a field strength of 5 mV/cm and a mobility
of 50 cm2/Vs and obtain |
|
|
| vD | = |
50 · 5 | |
mV · cm2 cm · V · s |
= 0,25 | cm s |
= 2,5 | mm s |
|
|
 |
That should come as some surprise! The electrons only have to move v e r y s
l o w l y on average in the current direction (or rather, due to sign conventions,
against it). |
|
 |
Is that true, or did we make a mistake? |
|
 |
It is true! However, it does not
mean, that electrons will not run around like crazy inside the crystal, at very high speeds. It only means that their net movement in current anti-direction is very slow. |
|
 |
Think of an single fly in a fly swarm. Even better read
the module that discusses this analogy in detail. The flies are flying around at high speed like crazy - but the fly
swarm is not going anywhere as long as it stays in place. There is then no drift velocity and no net fly current! |
| | |
© H. Föll (Electronic Materials - Script)