We now have hyperpure poly-Si, already doped to the desired level, and
the next step must be to convert it to a single crystal. There are essentially two methods
for crystal growth used in this case: |
|
 |
Crystals grown by the Czochralski
methodor crucible
grown crystals (CZ crystals). |
|
 |
Float zone or FZ crystals. |
 |
The latter method produces crystals with the highest purity, but is not easily
used at large diameters. 150 mm crystals are already quite difficult to make and nobody so far has made a 300
mm crystal this way. Float zone crystal growth, while the main method at the beginning of the Si age, is now
only used for some specialties and therefore will not be discussed here; some details
can be found in the link. |
|
 |
The Czochralski method, invented by the Polish scientist J. Czochralski in 1916, is the method of choice
for high volume production of Si single crystals of exceptional quality and shall be discussed briefly. Below is
a schematic drawing of a crystal growth apparatus employing the Czochralski method. More
details can be found in the link. |
|
|
|
|
 |
Essentially, a crystal is "pulled" out of a vessel containing liquid
Si by dipping a seed crystal into the liquid which
is subsequently slowly withdrawn at a surface temperature of the melt just above the melting point. There is a little trick
in doing that, that is the key to dislocation -free crystal growth and thus to all of microelectronics; see the link above. |
|
 |
The pulling rate (usually a few mm/min) and
the temperature profile determines the crystal diameter (the problem is to get rid of
the heat of crystallization). |
|
 |
Everything else determines the quality and homogeneity - crystal growing is still
as much an art as a science! Some interesting points are contained in
the link. |
 |
Here we only look at one major point, the segregation coefficient
kseg
of impurity atoms. |
|
 |
The segregation coefficient in thermodynamic equilibrium gives the relation between
the concentration of impurity atoms in the growing crystal and that of the melt. It is usually much lower than 1
because impurity atoms "prefer" to stay in the melt. This can be seen from the liquidus and solidus lines in the
respective phase diagrams. |
|
 |
In other words, the solubility of impurity
atoms in the melt is larger than in the solid. |
|
 |
"Equilibrium" refers to a growth speed of 0 mm/min or,
more practically, very low growth rates. For finite growth rates, kseg becomes a function of the growth
rate (called kseff) and approximates 1 for high growth rates (whatever comes to the rapidly moving
interface gets incorporated). |
 |
This has a positive and a negative side to it: |
|
 |
On the positive side, the crystal will be cleaner
than the liquid, crystal growing is simultaneously a purification method. Always provided that we discard the last part
of the crystal where all the impurities are now concentrated. After all, what was in the melt must be in the solid after
solidification - only the distribution may now be different. |
|
 |
This defines the negative side: The distribution
of impurities - and that includes the doping elements and oxygen - will change along
the length of a crystal - a homogeneous doping etc. is difficult to achieve. |
|
 |
That segregation can be a large effect with a sensitive dependence on the growth
rate is shown below for the possible doping elements; the segregation coefficients of the unwanted impurities is given in
a table. |
| |
| |
| Atom | Cu |
Ag | Au |
C | Ge |
Sn | |
| kseg |
4 · 104 |
1 · 106 |
2,5 · 105 |
6 · 102 |
3,3 · 101 |
1,6 · 102 |
| | Atom |
O | S |
Mn | Fe |
Co | Ni |
Ta |
| kseg |
1,25 |
1 · 105 |
1 · 105 |
8 · 106 |
8 · 106 |
4 · 104 |
1 · 107 |
|
|
 |
We recognize one reason why practically only
As, P, and B is used for doping! Their segregation coefficient is close to 1 which assures half-way
homogeneous distribution during crystal growth. Achieving homogeneous doping with Bi, on the other hand, would be
exceedingly difficult or just impossible. |
 |
Present day single crystals of silicon are the most perfect objects on this side
of Pluto - remember that perfection can be measured by using the second law of thermodynamics; this is not an empty statement!
A very interesting and readable article dealing with the history
and the development of Si crystal growth from W. Zulehner
(Wacker Siltronic), who was working on this subject from the very beginning of commercial Si crystal growth until
today, can be found in the link. |
|
 |
What the finished crystal looks
like can be seen in the link. What we cannot see is that there is no other crystal of a different material that even comes
close in size and perfection. |
|
 |
Our crystal does not contain dislocations - a unique feature that only could be
matched by Germanium crystals at appreciable sizes (which nobody grows or needs)1).
It also does not contain many other lattice defects. With the exception of the doping atoms (and possible interstitial oxygen,
which often is wanted in a concentration of about 30 ppm), substitutional and interstitial impurities are well below
a ppb if not ppt level (except for relatively harmless carbon at about 1 ppm) - unmatched by most other
"high purity" materials. |
|
 |
Our crystal is homogeneous. The concentration of the doping atoms (and possibly
interstitial oxygen) is radially and laterally rather constant, a feat not easily achieved. |
 |
The crystal is now ready for cutting into wafers. |
| |
|
Wafer Technology |
| |
|
|
It may appear rather trivial now to cut the crystal into slices which, after some
polishing, result in the wafers used as the starting material for chip production. |
|
 |
However, it is not trivial. While a wafer does not look
like much, its not easy to manufacture. Again, making wafers is a closely guarded secret and it is possibly even more difficult
to see a wafer production than a single Si crystal production. |
|
 |
First, wafers must all be made to exceedingly tight geometric specifications. Not only must
the diameter and the thickness be precisely what they ought to be, but the flatness is constrained to about 1 µm.
|
|
 |
This means that the polished surface deviates at most about 1 µm from an ideally
flat reference plane - for surface areas of more than 1000 cm2 for a 300 mm wafer! |
|
 |
And this is not just true for one wafer, but for all 10.000 or so produced daily in
one factory. The number of Si wafers sold in 2001 is about 100.000.000
or roughly 300.000 a day! Only tightly controlled processes with plenty of know-how and
expensive equipment will assure these specifications. The following picture gives an impression of the first step of a many-step
polishing procedure. |
|
|
 |
© "Smithsonian", Jan 2000, Vol 30, No. 10 Reprinted with general permission |
|
 |
In contrast to e.g. polished metals, polished Si wafers have a perfectsurface - the crystal just ends followed by less than two nm of "native oxide" which forms rather quickly in air and protects the wafer from chemical attacks. |
|
 |
Polishing Si is not easy (but fairly well understood) and so is keeping the surface
clean of particles. The final polishing and cleaning steps are done in a cleanroom where
the wafers are packed for shipping. |
|
 |
Since chip structures are always aligned along crystallographic directions, it is important
to indicate the crystallography of a wafer. This is done by grinding flats (or, for
very large wafer - 200 mm and beyond notches) at precisely defined positions. |
|
 |
The flats also encode the doping types - mix ups are very expensive! The convention
for flats is as follows: |
 |
Typical wafer specifications may contain more than 30 topics, the most
important ones are: |
|
 |
Doping type: n or p-type (p-type
is by far the most common type) and dopant used (P, As or B). Resistivity (commonly between 100 Wcm to 0,001 Wcm
with (5 - 1) Wcm defining the bulk of the business. All numbers with error margins and
homogeneity requirements |
|
 |
Impurity concentrations for metals and other "life
time killers" (typically below 1012 cm–3), together with the life
time or diffusion length (which should be several 100 µm). |
|
 |
Oxygen and carbon
concentration (typically around 6 · 1017 cm–3 or 1 · 1016 cm–3,
respectively. While the carbon concentration just has to be low, the oxygen concentration often is specified within narrow
limits because the customer may use "internal gettering", a process where
oxygen precipitates are formed intentionally in the bulk of the wafer with beneficial effects on the chips in the surface
near regions. |
|
 |
Micro defect densities (after all, the point defects generated
in thermal equilibrium during crystal growth must still be there in the form of small agglomerates). The specification here
may simple be: BMD
("bulk micro defect") density =0 cm–3. Which simply translates into: Below the detection
limit of the best analytical tools. |
|
 |
Geometry, especially several parameters relating to flatness.
Typical tolerances are always in the 1 µm regime. |
|
 |
Surface cleanliness: No particles and no atomic or molecular
impurities on the surface! |
 |
This link provides a grapical overview
of the complete production process - from sand to Si wafers - and includes a few steps not covered here. |
|
 |
Appreciate that the production of wafers - at last several thousands per day - with specifications
that are always at the cutting edge of what is possible - is an extremely involved and difficult process. |
|
 |
At present (Jan. 2004), there are only a handful of companies world wide that can do
it. In fact, 4 companies control about 80% of the market. |
 |
This link leads to a recent (1999) article covering new
developments in Si CZ crystal growth and wafer technology (from A.P. Mozer;
Wacker Siltronic) and gives an impression of the richness of complex issues behind the production of the humble Si
wafer. |
 |
This link shows commercial wafer
specifications. |
|
 |
To give an idea of the size iof the industry: In 2004 a grand total of about 4.000.000
m2 of polished Si wafers was produced, equivalent to about 1.25 · 108
200 mm wafers. |
© H. Föll (Semiconductor Technology - Script)