In reality, however, we have a dynamic equilibrium:
Electron–hole pairs are generated all the time and they recombine all the time, too – but their average density
in equilibrium stays constant. |
|
 |
The easiest way to include this dynamic equilibrium in the formal representation
of semiconductors is to introduce the concept of the minority carrier life time,
or life time in short. |
|
 |
Here we look at it in a extremely simplified way – the idea is to just get the fundamentals
right. In the next chapter we will delve a little deeper into the subject. |
 |
Let's consider a p-doped semiconductor. The majority
carriers then are holes in the valence band; in the appropriate temperature range, their density is essentially given
by the density of the acceptors put into the material. |
|
 |
The electrons in the conduction band are the minority carriers, their density ne
is given via the mass action law (nh ·
ne = ni2) by equating the majority carrier density with the density of the doping atoms:
|
| |
| ne | = |
nmin | = |
ni2 nh |
= | ni2
NA |
|
|
|
Now consider some light impinging on the material with an energy larger than the
band gap, so it will be absorbed by generating electron–hole pairs. Let's assume that Ghn
electron hole pairs will be generated every second (the index "hn" refers to
the photons via their energy to distinguish this generation rate from others
yet to come). |
|
 |
The density of both electrons and holes will now increase and no longer reflect the equilibrium
values. |
|
 |
The deviation from equilibrium is much more pronounced for the minority carriers (which here
are the electrons). If, for example, the density of the electrons is 0.1 % of the hole density; an increase of the
hole density of 0.1 % due to the light-generated holes would increase the electron population by 100 %. |
|
 |
Consequently, in non-equilibrium conditions, we are mostly interested in what happens to the
minority carriers – the majority carriers then will be automatically taken care of, too, as we will see. |
 |
Evidently, the density of minority carriers cannot grow indefinitely
while light shines on the semiconductor. Some of the excess electrons will disappear again due to recombination with holes. |
|
 |
If the recombination rate is proportional
to the density of the minorities, an equilibrium will be reached eventually, where the additional rate of recombination
equals the generation rate Ghn, and the density will then be constant
again at some higher level. |
|
 |
If we now were to turn off the light, the minority carrier density will decrease (in the usual
exponential fashion) to its thermal equilibrium value. The average time needed for a decrease of 1/e is the minority carrier life time
t. |
 |
This is a simple but nonetheless correct way to think about life times and we
are now using this concept to arrive at a few more major properties and relations. |
| |
|
Direct
and Indirect Semiconductors |
| | |
 |
First, let's consider the rough magnitude of the life time t.
A recombination process implies that the (quasi) wave vectors of both, electron and hole, change during this process –
simply because the particles annihilate each other, so also the (quasi) wave vectors get annihilated in the end. |
|
 |
Any change in (quasi) wave vector is always subjected to the requirement of conservation of
the (crystal) momentum. In the simplest case of a band–band transition, this requires a vertical line in the reduced band diagram. |
|
 |
This
is only possible if there are occupied electron and hole states directly on top of each other. Let's visualize this
by looking at the electron–hole pair generation process by a photon more closely: |
| |
|
|
 |
Shown is the band diagram for an indirect semiconductor, i.e. the minimum of the conduction
band is not directly over the maximum of the valence band. |
|
 |
A photon with the energy hn lifts an electron from somewhere
in the valence band to a position directly overhead in the conduction band, giving all its energy to the electron. That
the new state of the electron lies "directly overhead" is due to the fact that the momentum of the photon is neglibly
small. |
|
 |
Instant exercise: Show that this is true by estimating the magnitude
of the photon's wavevelength, l, for a photon energy of 1 eV. Why is it sufficient to
know this value? (Hint: We consider band–band transitions within the first Brillouin zone.) |
|
 |
A hole and an electron deep in the valence band or conduction band, respectively, are created
which immediately (within picoseconds), by releasing phonons, give up their surplus energy relative to the maximum of the
valence band or minimum of the conduction band, respectively, and thus come to an energetic rest at the extrema of the bands. |
|
 |
Their wave vectors now are different – direct recombination is not allowed; it would
violate Braggs (generalized) law or the conservation of crystal momentum. Recombination
needs a third partner (e.g. lattice defects), and life times will be large (typically
microseconds if not milliseconds) and depends somehow on the density of suitable third partners. |
|
 |
Did you look closely? Yes? Closely enough to notice that this picture contains
a very basic mistake (that doesn't influence what has been discussed, however)? Good! If you didn't notice, you may want
to activate the link. |
 |
For direct semiconductors the diagram would be very similar, except that the extrema
of the bands are now on top of each other. |
|
 |
Recombination now is easily possible, the energy liberated will be in the form of a photon
– recombination thus produces light. |
|
 |
Life times in the case of direct semiconductors thus tend to be short
– typically nanoseconds – and are dominated by the properties of the semiconductor itself. |
 |
What exactly determines the life time in indirect semiconductors like Si?
In our simplified view of "perfect" crystals, would recombination simply be impossible? |
|
 |
There are several mechanisms that make recombination possible in real crystals. Generally,
a third partner is needed to provide momentum conservation (and is thus also involved in the energy transfer). |
|
 |
Usually, this third partner is a defect of some kind. Most notorious are certain atomic defects,
often interstitial atoms as, e.g., Fe, Ni, Cu, Au, and many others. But the doping atoms and
coarser defects like dislocations and grain boundaries also help recombination along. Last, but also least, it is also possible
that phonons get involved. |
 |
In summary, the life time of indirect semiconductors is dominated
by defects, by impurities, by anything that makes the crystal imperfect. It is thus a property that can vary over many orders
of magnitude – some examples can be found in the link. In very
perfect indirect semiconductors, however, it is a very large time (for electrons), and can easily be found in the millisecond
range. |
| |
|
Generalization |
| | |
 |
In an important generalization of what has been said so far, we realize that a
minority carrier does not "know" how it was generated. Generation by a thermal energy fluctuation in thermal equilibrium
or generation by a photon in non-equilibrium – it's all the same! |
|
 |
The minority carrier, once it was generated, will recombine (on average) after the life time
t. This is valid for all minority carriers (at least as long as their density is not too
far off the the equilibrium value). |
|
 |
This implies that the minority carriers will disappear within fractions of a second after
they were generated! |
 |
However, since we have a constant density of minority carriers in thermal equilibrium,
we are forced to introduce a generation rate
G for them
that is exactly identical to their recombination rate
R
in equilibrium. |
|
 |
In other words, the carrier densities in the valence and conduction bands
are not in static, but in dynamic equilibrium (see the thermodynamics script as well). |
|
 |
Their (average) density stays constant as long as G = R. Think of your bank
account. Its average balance will be constant as long as the withdrawal rate is equal to the deposition rate. |
 |
From the values of the densities we can not make any statement as to the recombination
and generation rate – your bank balance stays constant if you withdraw and deposit 1 $ a week or 1 million
$! |
|
 |
If we know the life time t, however, we can immediately
write down the recombination rate: |
|
 |
R is the number of recombinations per second (and per cm3),
i.e. R = nmin/t
with nmin = density (or number; as always we use these quantities synonymously even so this
is not strictly correct) of minority carriers. |
|
 |
With the relations from above we obtain the following expression:
|
| |
|
| |
With NDop = density of the doping atoms. |
 |
This equation is a good approximation for the temperature range where the doping
atoms are all ionized but little band–band transitions take place, i.e., in the temperature range where the semiconductor
is usually used. And do not forget: it is only valid in thermodynamic equilibrium. |
| |
|
Diffusion Length
|
| | |
 |
Minority (and majority) carriers are not sitting still in the lattice (they are
only "sitting still" in k-space!), but move around with some average velocity. |
|
 |
In the free electron gas model this velocity could be directly
calculated from the momentum mv = ·k, so v = k/m. |
|
 |
But this is the
phase velocity and this relation does not apply to the holes and electrons at the edges of the valence and conduction
band, i.e. in the region of the dispersion relation where the differences between the free electron gas model and the real
band structure is most pronounced and the group velocity can be very low if not zero. |
|
 |
For the purpose of this subchapter let's simply assume that the carriers move randomly through
the lattice (being scattered all the time) and that this movement can just as well be described by a diffusion coefficient
D as always. |
|
 |
We already had a glimpse that there is a connection
between the mobility µ and the random movement of the carriers. Here we will take this for granted (we will
come back to this issue later) and take note of this simple,
but far-reaching relation, called Einstein
relation. This relation connects the mobility and the diffusion coefficient
D
via |
| |
|
|
 |
The diffusion coefficient D, of course, is the proportionality constant that
connects the diffusion current j of particles (not necessarily an electrical current!) to their density gradient
Ñr(x,y,z) (with r
= density of the particles) via Fick's
first law: |
| |
| j(x,y,z) | = – |
D · Ñr(x,y,z ) |
|
|
 |
Bearing this in mind, we now can relate the average distance (x2
+ y2 + z2)1/2 that a particle moved away from its position (0,0,0)
at t = 0 after it diffused around for a time t via another Einstein relation by |
| |
| <r > |
= | æ è |
D · t | ö ø |
1/2 | = |
æ ç è |
kT · µ · t
e |
ö ÷ ø | 1/2 |
|
|
|
 |
A minority carrier with a specific life time t
thus will be found at an average distance from the point were it was generated given by |
| |
| <r> |
= | æ è |
D · t |
ö ø | 1/2 |
=: | L |
|
|
|
 |
This specific distance we call the diffusion
length
L of the minority carriers.
|
 |
The diffusion length L is just as good a measure of the dynamics
of the carrier system as the life time t; we can always switch from one to the other via
the Einstein relations. |
|
 |
Long life times correspond to long diffusion lengths. In today's Si, diffusion lengths
of mm can be achieved – a tremendous distance in the world of electrons and holes. |
| | |
|
Real Semiconductors |
| | |
 |
So far we have explicitly or implicitly only considered "perfect" semiconductors
– i.e., semiconductors without any unintentional lattice defects. But now it is easy to consider real semiconductors.
Real semiconductors contain unintentional lattice defects and these defects can have two major detrimental effects if they
introduce energy levels in the band gap. |
|
 |
They may influence or even dominate the carrier density,
i.e. they act as unwanted dopants. In many cases of semiconducting materials without any technical applications so far,
the carrier density is pretty much determined by defects and is practically unalterable (it usually also comes in only one
kind of conductivity type). |
|
 |
They influence or dominate the minority carrier life time.
This may be a major problem, e.g. for solar cells where large life times are wanted in rather imperfect materials. |
|
 |
In addition, they will also influence the mobility (usually
decreasing it). |
 |
Technically, there are several options for dealing with real semiconductors. |
|
 |
Make the material very perfect. This is the recipe for Si microelectronics and most
of the III-V compound devices. |
|
 |
Live with the defects and render them impotent as far as possible, e.g. by hydrogen passivation. |
|
 |
Find semiconductors where the defect levels are not in the band gap (after passivation). An
example may be CuInSe2, which is usable for solar cells despite lots of defects, and GaN, which
is the standard material for blue light-emitting diodes. |