Chemical Vapor Deposition (CVD) is simple in principle |
|
Epitaxial Si layer
| | | |
| SiCl4 + 2 H2 |
Þ | Si + 4 HCl |
| | (1000 oC - 1200 oC) |
|
Polycrystalline Si layer
| | | | | | 60 Pa | |
| SiH4 | Þ
| Si + 2 H2 | | | 630oC
| |
SiO2 layer ("TEOS process)
| | | |
| Si(C2H5O)4 |
Þ |
SiO2 + 2H2O + C2H4 | | |
(720 oC) | |
Si3N4 layer
| | | |
| 3 SiH2Cl2 + 4NH3 |
Þ |
Si3N4 + 2HCl + 1,5 H2 | | |
(» 700 oC)) | |
W layer
| | | | | | 104 Pa |
| | WF6 + H2 |
Þ | W + (nasty) gases |
| | 470oC | |
|
|
|
 |
Find to gases that react ot the desired material at elevated temperatures |
|
|
 |
Put your wafer(s) into some machine, evacuate, heat to the desired temperature (preferably
only the wafers) and admit the gases (and remove undesired reaction products). |
|
|
 |
There are many quute different technical ways (all of them expensive) to realize a CVD
apparatus | |
|
| |
|
 |
Major CVD process are |
|
 |
Deposition of epitaxial Si layers - obviously always on (atomically clean)
Si substrates. By admitteing some gases carrying doping atoms (e.g. AsH3, AsH3) the
layer can be doped in-situ. | |
 |
Depositon of poly crystalline Si layers. |
|
|
 |
Chemically similar to epitaxial layers, in reality quite different because the CVD reactos
can be simpler. | |
|
 |
Poly-Si is needed for many uses: Gate electrode, interconnect, filling of holes, sacrifical layer.
| |
|
 |
Its great advantage is its ull compatibility with Si and SiO2; its
great disadvantage is its mediocre conductivity (for heavy doping). |
|
 |
Deposition of Si3N4 |
|
|
 |
Very important. Always prone to produce mechanical stress (Si3N4
is an unyielding ceramic!). | |
 |
W (and Silicides, and ...) |
|
|
 |
Not "good" processes, but sometimes unavoidable! |
|
|
|