Lets look at a simple cubic lattice containing one vacancy and connect the atoms by springs
symbolizing the bonds. It looks like this: |
|
| | |
|
| |
|
|  |
We have two kinds of springs:
- The red ones connect nearest neighbors and will heavily influence the vibration frequencies.
- The violet ones, connecting diagonally. They will have some bearing on the vibration frequency,
but since they must be weaker (the bond is weaker) than the red springs, their influence should be less pronounced.
|
 |
However, without the violet springs you could not make a stable crystal if you tried to built a model with
balls and springs. |
 |
Lets assign a spring constant D to the red springs and c · D to the violet
springs, with c < 1, and see what we get for the vibration frequency of an atom completely surrounded
by other atoms and for the atoms around the vacancy. |
|
| | |
|
 |
Generally, the resonance (circular) frequency w
of a particle with mass m is given by |
|
|
|
 |
In the most simple approximation, only accounting for the red springs, a regular
atom would feel the force of two springs per direction
and thus vibrate in any of the three dimensions with |
|
| . |
| |
|
 |
The six atoms (for three dimensions) surrounding the vacancy and missing one red spring each (in one dimension), in contrast, would vibrate in one of the three dimensions with
|
| |
|
 |
The entropy of formation SF then becomes (note that we
only have to sum over the "afflicted" dimensions): |
|
|
| SF | = |
k · | 6
S 1 |
ln |
w0
w1 |
= k · 6 · ln (2)1/2 = 3k · ln 2 = 3k · 0,693 |
| | | |
| | |
| | | = |
2,08 k |
|
|
 |
Not bad for such a simple approximation. But now lets go one step further and
add the violet springs. |
|
 |
We have now for the frequency of the lattice atoms without a vacancy |
| |
|
|
 |
and we simply include the factor (1/2)–1/2, that would give us the
component of the violet springs in the direction considered, into c; we thus have c < 0,707. |
 |
We now have to consider the 6 atoms with a missing red spring and 2
missing violet springs separately from the 12 atoms just missing one violet spring which are vibrating with w2, and consider the changed w0, too. Altogether we have
|
| |
| w02 |
= | 2D + 4cD
m | | | |
|
| w12 | = |
D + 2cD m |
| | | |
| w22 | = |
2D + 3cD m |
|
|
 |
The entropy now is |
|
|
| SF | = k · |
æ ç è |
6 S
1 | ln |
w0
w1 | + |
12 S
1 | ln |
w0
w2 |
ö ÷ ø |
|
|
|
 |
Crunching the numbers gives |
|
|
| SF | = |
3k · ln | 2 + 4c 1 + 2c |
+ 6 · ln |
2 + 4c 2 + 3c |
= 3k ·ln (2) + 6k · ln |
2 + 4c 2 + 3c |
|
|
|
 |
For c = 0 we must obtain our old result which indeed we do (check it), and for
c = 0,707, the most extreme case possible, we find |
|
|
| SF | = |
3k · ln (2) + 6k · ln (1,171) = 2,08 k + 0,947k = 3,027
k |
|
|
 |
In other words: For realistic c values, the correction is negligible
and we can confidently claim that the formation entropy of a monovacancy in a cubic primitive lattice is around 2 k
in our ball and spring model approximation. |
|
|